Originally Posted by Slipknot View Post
I used a 2 part finish that uses an acid catalyst. I had no time to use 2 part urethane like I wanted to since they could not wait the 21 days it would take for full cure and it would show scratches all over, so it was cheaper and quicker this way. They are happy and it looks great. I used commercial conversion varnish in satin for the rest of the furnishings.
We use conversion varnish quite a bit.

Did you use vinyl sealer under the cv?Some years back I refinished the mahogany table tops for a local restaraunt and the sample failed.The issue was that the owners wanted grain fill.Sprayed the cv straight over the fill and it flaked off.Come to find that I needed to use vinyl sealer over the fill.I now use it regardless because you never know.